PHYSICAL PROPERTY OF TEST DATA
|
| Material : |
CR 70 SHORE A (NEOPRENE 70) |
Date : |
FEB/21/2003 |
| Progum No. |
SC7051 |
Colour : |
BLACK |
| Spec: |
ASTM D2000 M3BC707A14B14EO14EO34 |
| Original Properties : |
Spec. |
Progum Data |
| Hardness, Shore A |
70
+/-5 |
72 |
| Tensile
strength, min, MPa |
7 |
17.2 |
| Elongation,
min, % |
200 |
278 |
| Specific
Gravity |
|
1.455 |
A1-14 Heat Resistance : 100ºC x 70
hrs
Test method D573 |
| Hardness Change, max, pts |
+ 15 |
-1 |
| Tensile Strength Change, max, % |
-15 |
-1 |
| Elongation Change, max, % |
-40 |
-6 |
B14 Compression Set : 100 ºC
x 22 hrs
Test method D395, Method B. |
| Max, % |
35 |
16.1 |
EO14 : ASTM #1 Oil : 100 ºC
x 70 hrs
Test Method D471. |
| Hardness Change, pts |
+/-10 |
-7 |
| Tensile Strength Change, max, % |
-30 |
-5 |
| Elongation Change, max, % |
-30 |
-16 |
| Volume Change, % |
-10 ~ +15 |
-13.4 |
EO34 ASTM #3 Oil: 100 ºC X 70
hrs
Test Method D471. |
| Tensile Strength Change, max, % |
-60 |
-28 |
| Elongation Change, max, % |
-50 |
-29 |
| Volume Change, max, % |
+100 |
-51.9 |
| Remark : |
1. |
The PROGUM data are based on testing slabs/buttons and are for
reference purpose only |
| |
2. |
PROGUM compound can meet above-mentioned ASTM D2000
spec. |
| |
3. |
This information is, to the best of our knowledge, accurate &
reliable to the date indicated. The above mentioned data have been
obtained by tests we consider as reliable. We do not assure that
the same results can be obtained in other laboratories, using different
conditions by the preparation and evaluations of samples. |
|