PHYSICAL PROPERTY OF TEST DATA
|
| Material : |
HNBR 80 SHORE A |
Date : |
DEC/09/2006 |
| Progum No. |
SH8054 |
Colour : |
GREEN |
| Spec: |
ASTM D2000 M3DH810A26B16B36EO16EO36 |
| Original Properties : |
Spec. |
Progum Data |
| Hardness, Shore A |
80
+/-5 |
85 |
| Tensile
strength, min, Mpa |
10 |
23.82 |
| Elongation,
min, % |
175 |
208 |
| Tear
Resistance, Kg-cm |
|
48 |
| Modulus
at 100%, MPa |
|
14.15 |
| Modulus
at 200%, MPa |
|
23.51 |
| Specific
Gravity |
|
1.485 |
A26 Heat Resistance : 150ºC x 70
hrs
Test method D573 |
| Hardness Change, max |
+ 10 |
+3 |
| Tensile Strength Change, max, % |
-25 |
0 |
| Elongation Change, max, % |
-30 |
-14
|
B16 Compression Set : 150ºC
x 22 hrs
Test method D395, Method B. |
| Max, % |
30 |
11 |
B36 Compression Set : 150ºC
x 22 hrs
Test method D395, Method B. |
| Max, % |
50 |
21 |
EO16 ASTM #1 Oil : 150 Cº x
70 hrs
Test Method D471. |
| Hardness Change, max |
-5~+10 |
+1 |
| Tensile Strength Change, max, % |
-20 |
+5 |
| Elongation Change, max, % |
-30 |
-12 |
| Volume Change, % |
+/-5 |
-2 |
EO36 ASTM #3 Oil : 150 º C x
70 hrs
Test Method D471. |
| Hardness Change, max |
-15 |
-7 |
| Tensile Strength Change, max, % |
-30 |
-6 |
| Elongation Change, max, % |
-30 |
-17 |
| Volume Change, % |
+25 |
+12 |
|
Low Temperature Test
-30 ºC x 3 min.
|
No Crack |
PASS |
| Remark : |
1. |
The PROGUM data are based on testing slabs/buttons and are for
reference purpose only |
| |
2. |
PROGUM compound can meet above-mentioned ASTM D2000 spec. |
| |
3. |
This information is, to the best of our knowledge, accurate &
reliable to the date indicated. The above mentioned data have been
obtained by tests we consider as reliable. We do not assure that
the same results can be obtained in other laboratories, using different
conditions by the preparation and evaluations of samples. |
|